Sažetak

Background and purpose
The aim of the work was to compare the interactions of three newly synthesized non-toxic starch derivatives, with varied anionic and non-ionic functional groups with methylene blue (MB) as a model cationic drug, and selection of starch derivative with highest affinity to the MB.
Experimental approach
The native potato starch (SN), modified via acetylation (SM1), esterification and crosslinking (SM2) and crosslinking (SM3), was evaluated in MB adsorption studies and assessed by FTIR, PXRD, and DSC.
Key results
The adsorption of MB on SM2 and SM3 matched the BET isotherm model, which confirmed physisorption on the low-porous surface. In the case of SM1, adsorption took place via electrostatic attraction between the heterogeneous adsorbent surface and the adsorbate, as demonstrated by the Freundlich plot. The FTIR confirmed vibrations assigned to N=C stretching bonds at 1600 cm-1 in the case of MB adsorbed on the SN and SM2. The most intense PXRD peaks belonged to SN and the least to SM2. In the DSC study, the thermal stability via ΔT was assessed, with SM2 of lowest ΔT value (179.8 °C).
Conclusion
SM2 presented the best adsorption capacity, followed by SM3 and the weakest SM1. The interactions were confirmed in the adsorption studies and may reflect applications of the modified starches as drug carriers. In the FTIR study, a probable interaction between the OH- groups of SM2 and N+ of MB was revealed. The most amorphous structure was shown for SM2, which was correlated with the lowest thermal stability provided by the DSC study.

Ključne riječi

potato starch; adsorption; interaction; methylene blue

Hrčak ID:

308784

URI

https://hrcak.srce.hr/308784

Datum izdavanja:

21.9.2023.

Posjeta: 464 *




Introduction

There are numerous newly developed carriers for therapeutic substances [1-3]. They are often completely new synthetic polymers [4,5]. Among polymers of plant origin, there are natural examples of potential carriers [6-10]. Wheat, maize and potato starch are available in large quantities from natural sources [11-13]. So far, starch has been modified by Utomo, Odeniyi, Singh et al. [14-16], among others. Previous publications have presented new methods for obtaining a number of starch derivatives [17-19] and proposed the potential use of some of them, including acetylated starch [20,21] and starch citrate [22]. The figure below shows the structural models of the modified potato starches created by the team from the University of Environmental and Life Science (Wrocław, Poland) (Figures 1a,b,c).

Some drugs have a 1,4-thiazine ring, which is included in the structure of methylene blue (MB). The study that used the similarity between MB and other molecules was performed on acridine and phenothiazine derivatives for anti-prion therapy [23]. Selected drugs include the 1,4-thiazine ring: phenothiazine, which has antiparasitic, antiseptic and antioxidant effects [24], promethazine, which has antihistamine and anti-allergic effects [25], chlorpromazine and [26] thioridazine - as psychotropic drugs. The ionic interaction between the promethazine and Eudragit® was ascribed to the electrostatic interaction between the drug and ammonium groups in the polymer backbone [27]. The interactions of chlorpromazine with cyclodextrin were realized via ionic bonds between the ionized amine group of chlorpromazine and anionic group of cyclodextrin sulfate [28]. Another study, which exploited cyclic voltammetry, interpreted the interactions of chlorpromazine and thioridazine with bovine serum albumin nanoparticles as a result of hydrophobic interaction [29]. Therefore, research has been undertaken on MB as a model drug representing the structural features of some active pharmaceutical ingredients (API). These studies may determine whether similar drugs could adsorb on modified starch. To date, studies have analyzed the adsorption of MB and other dyes on activated carbon, minerals of natural origin such as perlite, clay and its derivatives, bentonite [30,31], and agricultural solid wastes [32]. In summary, the important group that led to the intermolecular activity may be the ammonia group, which specifically interacts with anionic functionals. Because of the wide potential application of modified potato starch [33-36], we decided to compare the adsorption capacity of selected starch derivatives, characterized by a distinct negative charge of carboxyl and phosphate groups, or a characteristic ester group, towards methylene blue as a cationic substance.

The aim of the work was the evaluation of the prospective pharmaceutical applicability of three newly synthesized non-toxic starch derivatives, assessed via analysis of interactions of the starches, modified by varied acidic and non-ionic functional groups, with methylene blue, as a model cationic drug. The main question was the selection of the starch derivative with the highest affinity to the MB molecule. The possible interactions were evaluated in the terms of spectroscopic structural studies, as well as thermal assessments. The interactions, which may lead to drug release prolongation, were practically confirmed in the adsorption studies, which may reflect use of the above-mentioned modified starches as drug carriers for topical application, with retardant and prolonging effect against drug release process.

Materials

The following materials were employed in the study: methylene blue (MB, Reko, Dzierżoniów, Poland) - a model active pharmaceutical ingredient (API), native potato starch (SN) (PPZ, Niechlów, Poland), modified potato starches (starch acetate - SM1, starch citrate - SM2 and starch diphosphate - SM3) prepared according to below-described methods.

Methods

Preparation of the modified starches

The thermal and chemical modifications of native potato starch were conducted and resulted in acetylation (SM1), esterification and crosslinking (SM2), and crosslinking (SM3).

Preparation of acetylated starch (SM1)

The fractions of starch particles with an average volume moment diameter D [3,4] equal to 39.1 and 61.7 μm were separated from the native potato starch (SN) by measuring the volume diameter (Malvern laser particle size analyzer). Larger starch particles were acetylated with acetic anhydride in the amount of 13 cm3 /100 g of starch. After drying the acetylated starch, an initial gelatinization temperature of 49.17 °C was determined by differential scanning calorimeter Flash DSC (Mettler Toledo, Poland). The acetylated starch has been stirred for 24 h at 48 °C. It was then washed three times with five-liter portions of distilled water and separated from the slurry using the Contifuge Stratos (Heraeus, Germany) flow centrifuge. The obtained starch was dried for 24 h in an air dryer at 30 °C.

Preparation of citrate starch (SM2)

Native potato starch (SN) was esterified with citric acid. 10 g of citric acid per 100 g of starch dry matter was dissolved in 90 mL of water and thoroughly mixed. The resulting starch paste was left for 12 h at room temperature and then dried in an air dryer (Memmert, Germany) at 50 °C for 12 h. The starches were calcined for 3 h at 100 °C. The sample was rinsed three times with ethyl alcohol with a concentration of 95 mL of ethanol per 100 mL of solution, and each time, the solution was poured over the sediment. The washed precipitate was dried in an air dryer at 30 °C for 12 h. The obtained citrate starch was hardened at a temperature 2 degrees below the gelatinization temperature (determined by DSC), dried in an air dryer at 30 °C, ground in a laboratory mill and passed through a sieve with a mesh size of 400 μm [17].

Preparation of diphosphate starch (SM3)

Native potato starch (SN) (94.6 wt.%), sodium trimetaphosphate (1.2 wt.%), sodium carbonate (2.1 wt.%) and sodium chloride (2.1 wt.%) were introduced into the reaction vessel, 500 mL of distilled water at 45 °C was added. The mixture was adjusted to pH 10.5 with a 3 % NaOH solution. It was kept at 45 °C for 30 minutes with constant stirring, then neutralized with 8 % HCl to pH 6.5-6.8. The cross-linked starch was washed several times with distilled water on a funnel under vacuum and dried for 48 h at 25 °C. After obtaining starch diphosphate, it was hardened for 24 h at 2 degrees below the gelatinization temperature, dried in an air dryer at 30 °C, milled and sieved through a sieve with a mesh size of 200 μm.

Determination of the potential number of functional groups of modified starches

Based on the recipe for preparing individual modified starches, the mass values of substrates attached to native starch (SN), such as acetic anhydride, trimethaphosphate and citric acid, were converted to moles. The converted values per gram of SN are given inTable 1.

Spectroscopic evaluation

Fourier transform infrared spectroscopy (FTIR)

Fourier-transform infrared spectroscopy (FTIR) and attenuated total reflectance (ATR) appetizer (Nicolet 380 FTIR, Thermo Scientific, Waltham, MA, USA) with OMNIC ™ software were used to determine possible interactions between MB particles and starch. The formulations of MB adsorbed on every 50 mg of starch (SN, SM1, SM2 and SM3) were dried at 40 °C and compared with a physical mixture of MB and starch in a weight ratio of 1:10 and with the standards of the pure substances. The spectra of powders were recorded at wavelengths of 400 to 4000 cm-1 at 32 scans per sample and a resolution of 4 cm-1.

Powder X-ray diffraction (PXRD) analysis

The analysis of starch was supplemented by X-ray diffraction measurements (PXRD). The powder PXRD data were recorded on a Bruker D2 PHASER diffractometer (Bruker AXS, Karlsruhe, Germany) with a Lynxeye detector using Cu Kα radiation (0.15418 nm). All samples were measured at 295 K with 3.0 mm slit and 1.0 mm shutter. Diffractograms were obtained between 7.5° and 40° (2) (step size of 0.02° (2) and 0.25 s per step). The X-ray generator operated at 30 kV and 10 mA. The PXRD patterns were processed using the software Diffrac.Eva V 3.2. (Bruker AXS). The percentage of crystallinity and amorphousness of the tested starch samples in relation to SN was determined.

Thermal analysis

Differential scanning calorimetry (DSC)

Differential scanning calorimetry (DSC 214 Polyma, Netzsch, Selb, Germany) was performed to investigate the samples of dried adsorbed MB on 50 mg starches (SN, SM1, SM2, SM3), their physical mixtures of 1:10 w/w and pure ingredients. The grated samples of 3 to 5 mg were explored in aluminium pans with lids under a nitrogen atmosphere, with a flow rate of 50 mL min-1. The thermograms were recorded at a constant heating rate of 5 °C min-1 in the temperature range from 0 to 350 °C.

Evaluation of the adsorption kinetics of MB on the modified starches

The absorbance study was performed using four 50 mL conical flasks (A, B, C, D) as a series. 40 mL 6 mg L-1 MB was added for each flask. The SN, SM1, SM2 and SM3 starch probes of 2, 5, 10, 25, 50, 125, 250, 500, 750 and 1000 mg were placed in the flasks during the series, respectively. The flasks were put on the orbital shaker (at 100 rpm) at 22±0.5 °C. Four measurements of absorbance were proceeded based on the pharmacopoeial method by sampling the MB solution volumes of 3 mL in every 5, 10, 15, and 20 minutes, and than in equal periods up to 4 h. The solution was returned to the flasks. Analysis of taken samples was done by the spectrophotometer UV/VIS Jasco V-530 (Tokyo, Japan) at 663 nm, according to the available bibliography [37-39], and compared to the absorption spectrum of MB. A standard curve based on three series of measurements with five concentration points from 0.5 to 5.0 mg L-1 was prepared. The results were examined according to pseudo-zero-order kinetics and first-order kinetics. ANOVA statistical test was performed for independent groups at the significance level α = 0.05. Freundlich, Langmuir and BET isotherm models were taken for analysis of adsorption processes (Table 2). BET isotherm equation was adapted to form BET isotherm for liquid phase adsorption [40], where kBET(s) applies to the equilibrium constant of adsorption of the first layer and kBET(L) refers to the equilibrium constant of adsorption of upper layers.

The values of q and qt were calculated by the equations (1) and (2):

(1)
ADMET-11-1950-e001.jpg
(2)
ADMET-11-1950-e002.jpg

where C0 is initial concentration of the solution (mg L-1), Ct is concentration of the solution in time t (mg L-1), V is volume of solution (L) and m is adsorbent mass (g).

Equation (3) was used for the adsoprption (%) calculation:

(3)
ADMET-11-1950-e003.jpg

where m0 - the initial mass of the adsorbate, mt - is the adsorbate mass after time t.

Determination of the effect of MB adsorption on the pH of starch

The effect of MB adsorption on starch pH was investigated. The suspensions of pure starch in distilled water and suspensions of starch with adsorbed MB were prepared according to adsorption conditions (50 mg starch per 40 mL of water). pH measurements were taken after 1 and 72 h at 22±2 °C. Each measurement was taken three times. An ANOVA test with α = 0.05 was performed for these measurements.

Results

The results of the starch synthesis procedures yielded products with structures that conformed to the patterns (Figure 1 in the Introduction), and the appearance was as shown inFigures 2A and2B.

The molar ratio of functional groups added to the modified starches was converted per 1 g of native starch.

Spectroscopic evaluations

FTIR spectroscopy

The FTIR spectrum of pure MB showed a broad peak from 3219 to 3364 cm-1, indicating an O-H bending bond. The sharp peaks at 3050 cm-1 and in the range of 817 to 884 cm-1 were responsible for the presence of C-H or =C-H bonds in the aromatic ring. Similarly, a sharp peak around 2700 cm-1 may have occurred due to the C-H stretching bonds [41].

Characteristic peaks interacting at 1596 cm-1 might have been assigned to N=C stretching bonds. The peaks in the range 1420-1490 cm-1 most likely belonged to the stretching C=C-C bonds in the aromatic ring. Vibration from 1340 to 1360 cm-1 revealed the presence of C-N stretching bonds in aromatic tertiary amine [41] and peaks from 1059 to 1064 cm-1 and 661 cm-1 are related to C-S-C stretching bonds in heterocycle [42]. The pure starches FTIR spectra indicated a broad peak of O-H stretching bond at about 3300 cm-1, C-O stretching vibration at the range 1185-1347 cm-1, especially the strong peak at 1240 cm-1 for SM1 (Figure 3 b), C-O stretching bond at 930 cm-1 [43] and O-H bending bond at 988 cm-1 [44] (Figure 3).

The plot of the spectrum of adsorbed MB on the starch (red line) mostly followed the plot of the spectrum of the respective starch in its pure state (green line). However, there were locations where individual peaks were in excess. The peaks assigned to N=C stretching bonds at about 1600 cm-1 appeared in the case of MB adsorbed on the SN and SM2, however, to a very slight extent (Figure 3 a,c). The peak indicating the presence of the C=O bond of the acetyl group at 1730 cm-1 [45] was spotted on the SM1 spectra (Figure 3b).

PXRD

Diffractograms of modified starches were compared to those of SN (Figure 4). The peaks with the highest intensity were in the 2 range from 17.2 to 17.4°. The most intense belonged to SN and the least to SM2.

The proportion of crystallinity and amorphousness for the tested samples was determined using the amorphous subtraction method [46,47] and presented inTable 3.

Thermal properties

DSC analysis results shown inFigure 5 compared pure MB and evaluated starches with adsorbed MB and physical mixtures of these components. The thermograms showed the results of heat flow measurements from 0 to 350 °C taken in two cycles, with a cooling interval in between. The exothermic direction has been marked with an appropriate arrow (exo).

The results of DSC testing of native and modified starches under two heating cycles are shown inFigure 6.

The glass transition midpoint temperatures Tg, the difference in the heat capacity between the transition from glass to the liquid state ΔCp and ΔT - difference between onset crystallization temperature and Tg were analyzed using Proteus 7.0 software (Netzsch, Selb, Germany). The results are shown in theSupplementary material, Table S1.

Adsorption tests

The graphs showing the course of MB adsorption on starch showed the lowest saturation for SN and the highest for SM2 for 2 mg starch samples. It was 7.60 mg g-1 for SN and 22.86 mg g-1 for SM2 (Figure 7).

The amount of adsorbed MB increased with the enhancement of the mass of starch samples. The parameter values, adjusted to the tested kinetics models, based on the correlation factor, are given in theSupplementary material, Table S2.

Table 4 exhibits the parameters adapted to the chosen isotherm models. The samples of the starches were divided into two categories dependent on the mass; “A” was between 2 and 125 mg and “B” was between 250 and 1000 mg. Freundlich isotherm described in a satisfactory way adsorption equilibriums of MB adsorbed on the SN A, SM1, SM2 and SM3 B. The Freundlich exponent 1/n between 0.5723 and 0.9221 for SN “A” and SM1 “B” indicated favorable adsorption for which 1 ≤ 1/n. The adsorption on SM2 “B” had the largest value of kF. The adsorption on SM1 “A” had the lowest kF-value. In the case of the Langmuir isotherm, only SM2 “B” and SM3 “B” gave a satisfactory value of r2. However, in this case, the values of qm and kL were negative. The largest r2 values for the BET isotherm belonged to SM2 “B” and SM3.

Determination of the effect of MB adsorption on the pH of starch

The pH of starch suspensions with adsorbed MB compared to that of pure starch suspensions was higher for SM2 and lower for SN and SM1. In addition, there was a proportional increase in pH values after 72 h (Figure 8).

No significant differences were observed between the pH values of SN-MB and SM1-MB after 1 h (Figure 8a).

Discussion

Spectroscopic evaluations

FTIR spectroscopy

Due to the appearance of peaks at 1599 cm-1 assigned to the C=N bond on the FTIR spectrum of samples of adsorbed MB on SN and SM2, we postulate the existence of an interaction between the N+ ion derived from MB and the OH- group belonging to starch, which probably leads to enhanced adsorption of the dye on the polymer. This observation coincides with the mechanism of MB adsorption on black olive stone carried out by Al-Ghouti et al. [48].

PXRD

According toTable 3, the SN was the most crystalline, and SM2 the least. The crystallinity of SM increased according to the following pattern, SM2<SM3<SM1<SN, which suggests that the implementation of ionic groups resulted in the highest amorphicity, whereas the non-ionic acetyl groups in the lowest extent influenced the increase of amorphicity. This remark agrees with the results of Bhargav et al. [49], who assessed the combination of PVA with NaI. As the salt content of the polymer increased, the DSC diffraction peaks became less intense. They suggested high susceptibility of the amorphous structure of the polymer to ionic diffusivity of ionic particles. Similarly, Hodge et al. [50] found a correlation between peak intensity and the degree of crystallinity. They observed that the addition of water resulted in a decrease in XRD peak intensity and an increase in PVA amorphousness.

Thermal evaluation

DSC

The DSC thermograms of pure MB in the first heating cycle displayed an endothermic peak at about 80 °C responsible for the dehydration (Figure 5 a-d). The thermogram of the second heating cycle no longer showed this peak, while an endothermic peak in the 100 °C range appeared (Figure 5 e-h). MB forms several hydrates. In addition, it reacts with an aluminum container for DSC [51]. This endothermic peak may indicate a transition from one form of MB hydrate to another. In the thermogram of the first heating cycle, it was most likely obscured by the broad peak of dehydration. These speculations are confirmed by the shifted exothermic peaks occurring at 171 and 233 °C in the first heating cycle (Figure 5 a-d) and 201 °C in the second cycle (Figure 5 e-h). They testify to the decomposition of MB [52]. Omer et al. [53] indicated the occurrence of oxidation of MB at 260 °C. A difference was observed between the spectrum of adsorbed MB and physical mixed MB. An exothermic peak appeared, indicating the presence of MB in the physical mixture with SN (177.6 °C), SM1 (175.9 °C), SM2 (174.0 °C) and SM3 (177.2 °C) (Figure 5 a,b,c,d respectively). No MB peak was observed in MB adsorbed at SN and SM1 (Figure 5 a,b), which may indicate the absence or complete decomposition of MB. For MB adsorbed on SM2 and SM3, the course of these peaks was flattened at 174.4 and 176.7 °C, respectively, which may indicate the interaction of MB with these starches (Figure 5 c,d).

Glass transition temperature Tg value readings showed the lowest Tg for SM2 (47.2 °C) and the highest for SM3 (55.9 °C) (Table S1). Hydrogen bonds are among the factors affecting Tg [54]. Taylor et al. [55] observed significantly lower Tg of sucrose compared to other disaccharides. This was due to the less extensive hydrogen bonding network in the amorphous state. Similarly, Zhou et al. [56] demonstrated the dependence of Tg on hydrogen bonds occurring between polymer and copolymer particles (maleimide-isobutene alternating copolymers). A network of hydrogen bonds of carboxyl groups resulted in a higher Tg value than hydrogen bonds between hydroxyl groups. The lowest Tg occurred in the absence of hydrogen bonds between polymer molecules. In our case, the holders of the hydroxyl groups were SN and SM1 (Tg 52.2 and 51.15 °C respectively) (Table S1) and the carboxyl groups were present in the SM2 molecule. In addition, phosphate groups appeared in the SM3 molecule. High Tg values for SM3 may suggest the self-association of these starch molecules, whose Tg decreased to 53.0 °C after bond formation with MB [55]. In the case of SN, Tg values increased after MB adsorption (54.7 °C), what may indicate low self-association of SN particles in the pure state.

In the present work, the values of ΔT were assessed to determine the thermal stability of the tested samples. The higher the value of ΔT, the better the thermal stability. The value for SN was the highest (221.07 °C), demonstrating the highest thermal stability of this starch. At the same time, its highest percentage of crystallinity was confirmed (Table 3). On the contrary, SM2 showed the lowest value of ΔT (179.8 °C) - the lowest thermal stability. Keshk et al. [43] demonstrated the dependence of thermal stability on ΔT-values, which correlated with the degree of crystallinity of corn starch-cellulose mixtures, depending on the mixture ratio. They found an inversely proportional relationship between ΔT values and ΔCp values. Our ΔCp studies confirmed such a relationship outside of the SM2 samples having the lowest ΔCp value (0.465 J g-1·K-1) according to the lowest ΔT (Table S1). This phenomenon may be supported by the observation of Liu et al. [57]. They studied various starches whose structure was more or less amorphous. According to them, amorphousness gives the compounds a liquid-like structure. More amorphous compounds have a less ordered structure than those with a crystalline structure. They showed that the process of lowering the temperature below Tg leads to the reorganization of the structure. In our study, SM1, SM2 and SM3 starches were hardened at 2 degrees below Tg. Moreover, the research is confirmed by PXRD studies, where SM2 had the highest degree of amorphousness (Table 3).

The thermograms of the second heating cycle can show the structure of the compound when structural reorganization occurs after the cooling cycle. In the case of SM2 there was an endothermic peak at 215 °C, from which an increase in heat flow is observed. The thermograms of adsorbed MB on starches are characterized by different temperatures of the start of the exothermic process. The increase in heat flow started fastest for SM2_MB (adsorbed) at 157 °C and slowest for SM3_MB (adsorbed) at 163 °C (Figures 5g and5h, respectively). This endothermic event might be attributed to reduced hydrogen bonding as well as the interference of molecular organization due to the interaction between SM2, SM3 and MB. For SN_MB (adsorbed) and SM1_MB (adsorbed), no increase in heat flow was observed (Figures 5e and5f).

Adsorption tests

MB adsorption on starch predominantly matched a pseudo-second-order model. A study by Lin et al. [58] of MB adsorption on activated carbon indicated a better pseudo-second-order fit to both linear and nonlinear models. Similarly, Ma et al. [45] matched the adsorption of heavy metal ions on modified potato starch to the pseudo-second-order model. In our study, the highest k2 values obtained for SN, SM3, SM2 and SM1 were 1.9623, 1.5367, 0.9240, 0.1848 g mg-1·min-1, respectively, and occurred at a weight of 1000 mg for SN and SM1 and 2.0 mg for SM2 and SM3 (Table S2). This suggests that MB adsorbed fastest on SN, but this was dependent on the surface area of the adsorbent: the larger the surface area, the faster the saturation. In the case of SM2 and SM3, MB adsorbed fastest already on the smallest starch particle, suggesting a high affinity of the adsorbate to the adsorbent. The slowest adsorption was observed in SM1.

The q values in Table S2 differ from qm obtained according to Langmuir and BET isotherms. Moreover, some of the Langmuir adsorption constants (qm and KL) showed negative values (Table 4). Langmuir isotherm is known to get different parameters according to the calculation method [59-61], therefore, we used the course of the isotherm of MB on the starches to establish qm values (Figure 9).

Methylene blue is a substance that has been thoroughly studied by scientists because of its harmfulness to the environment. As a dye used in industry, it leaks into water waste in large quantities. Their purification is a major challenge for researchers. Many study substances that are adsorbents for MB and can serve as filters [32,61-65]. Some of these include starches and other polysaccharides.Table 5 shows the qm values of example adsorbents for MB.

The sigmoidal course of the SM2 and SM3 starch isotherms falls into type IV according to the IUPAC classification. SN and SM1 isotherms are more aligned with type VI [76]. Type IV represents single and multilayer adsorption plus capillary condensation. Type VI illustrates that the adsorption isotherm can have one or more steps. In our study, the adsorptions on SN and SM1 starches best fitted to the Freundlich isotherm model. On the other hand, for SM2 and SM3 starches, the adsorption courses more closely matched the BET isotherm (Table 4).

The Freundlich model describes multilayer adsorption on a surface, with an inhomogeneous distribution of binding sites and, therefore, an inhomogeneous energy distribution. The constant kF expresses the maximum adsorption on the surface of the adsorbent. The BET isotherm describes the phenomenon of physisorption on a non-microporous surface. The constant kBET is related to the adsorption energy. Bhattacharyya et al. [36] found graphene oxide-potato starch almost perfectly fitted to the Freundlich isotherm model. Dipa et al. [37] adapted MB adsorption on kaolinite to the Langmuir model. Bestani et al. [62] studied MB adsorption on carbon-activated leaves, which they fitted to the Langmuir and Freundlich models. El Qada et al. [31] matched MB adsorption on activated carbon to Redlich-Peterson and Langmuir isotherm models. The Redlich-Peterson model is a compilation of the elements in the equations of the Langmuir and the Freundlich isotherms. Langmuir isotherm mostly applies to chemisorption on a monolayer. Activated carbon is highly porous and is a well-known adsorbent used in industry as a filter [77]. The dependence of the isotherm model on the structure of the adsorbent can also be supported by the study of Ma et al. [45], who used potato starch modified with high temperature to increase its porosity. Adsorption of heavy metal ions on such modified starch showed good adherence to the Langmuir model. In the case of our experiment, only SM2 was subjected to high-temperature modification at 100 °C. This could most likely increase its adsorption properties.

Determination of the effect of MB adsorption on the pH of starch

The measured pH and pKa values of the acids from the literature enabled us to estimate the number of moles of functional groups derived from the molecules and finally present at the modified starches. The calculated values are gathered inTable 6.

The initial assumptions of the ratio of the number of millimoles of functional groups on the modified starches used to react with the native starch during its modification was 23:13:1 for SM1:SM2:SM3, respectively (Table 1). The millimole ratio of the same groups, calculated from the pH values of the modified starch suspensions after 1 h, was 1:13:0.03. This shows that the activity of acyl and phosphate groups decreased 23 and 33 times compared to carboxyl groups, respectively. MB solution with pH of 4.26 resulted in the acidification of SN and SM1 suspensions. It did not change the pH for SM3. The increase in the pH value of the suspension of adsorbed MB on SM2 starch may indicate the most effective binding of MB to the carboxyl groups of SM2 (Figure 9).

Effect of type of functional groups of modified starches on interactions with MB

The MB adsorbed on the 1000 mg of the starch decreased according to the following pattern: SN > SM2 > SM3 > SM1 (Figure 7). The hydroxyl, carboxyl and phosphate groups of starch favored MB binding to the polymer to the greatest extent, while the acetyl groups had the greatest effect on the reduction of adsorption capacity. The rationale for the decreased sorption capacity could be the blocking of starch functional groups in the structure of starch polymer or the specific activity of functional groups towards MB. Dipa et al. [37] observed the effect of NaOH-derived hydroxyl groups on the increase of MB adsorption on kaolinite. However, these were groups added to kaolinite. In our case, only the carboxyl, phosphate and acyl groups originated from acids and were added during the starch modification process. Physisorption may be taken into account in the case of SN and SM3. It differs for SM2 and SM1, where acid groups can affect MB adsorption. Similar conclusions were issued by Huang et al. [80] after studying the adsorption of Pb2+ ions on activated carbon with additional functional groups. Pb2+ ions were adsorbed according to three mechanisms: (1) in mesopores, (2) via bonds between -OH and C=O and Pb2+, (3) H+ from the acidic carboxyl and phosphate groups is replaced by the Pb2+ ion.

An additional element worth highlighting is the effect of the method of preparation of modified starches on their structure. Two of our SM2 and SM3 starches were prepared using the crosslinking method, which provides increased starch stabilization by forming bridges between hydroxyl groups and anhydroglucoses [81]. Kapelko et al. [17] found crosslinking reactions caused a decrease in solubility in water and a decrease in phase transition. Shen et al. [82] used corn starch and citric acid, malic acid, succinic acid and 1,2,3,4-butanetetracarboxylic acid (BTCA) as cross-linkers. They observed that the acid with more carboxyl groups (citric acid and BTCA) showed higher crosslinking degrees and enhanced mechanical properties than acids with two carboxylic groups. Moreover, as they are used in food modification, poly-carboxylic acids are in the category of safe chemicals [83]. In the case of SM1 and SM3, the chemically modified starches with a low degree of substitution (DS) are permitted for use in the food industry and are denoted with the symbol “E” followed by an appropriate number. Among others, acetylated starch (E1420) and di-starch phosphate (E1412) belong to this group [84].

Conclusions

Citrate starch (SM2) presented the best adsorption capacity, followed by phosphate starch (SM3), and acetylated starch (SM1) showed the weakest adsorption capacity, according to the adsorption results. MB adsorption on SM2 and SM3 followed the BET isotherm model, which shows the physical adsorption of the cationic dye on the low-porous surface. In the case of SM1, MB adsorption probably took place via electrostatic attraction between the heterogeneous adsorbent surface and the adsorbate molecules, as indicated by the Freundlich adsorption model.

Spectral methods confirmed the adsorption capacity of SM2. In the FTIR study, a probable interaction between the OH- groups of SM2 starch and N+ of MB was revealed on the basis of characteristic vibration of the C=N bond in the adsorbent derived from MB at 1600 cm-1.

The DSC results showed the lowest thermal stability of SM2 correlated with its amorphous structure. Moreover, according to DSC, the possibility of interaction between SM2 or SM3 and MB was demonstrated via the existence of an exothermic peak belonging to MB in samples of these two adsorbents. The appearance of endothermic peaks in the case of SM2 and SM3 samples with adsorbed MB in the second heating cycle confirmed the interaction between the adsorbents and the adsorbates. The effect of the manufacturing method of the modified starches on their durability was noted. SM2 and SM3 starches were prepared using the crosslinking method, which provided increased starch stabilization.

The above presented properties and, in addition, the “safe chemistry” and slightly acidic pH of the tested starches make them useful, especially citrate starch, as carriers for biologically active substances containing cationic groups, in topical skin applications. The present research confirms our previous studies on lidocaine hydrochloride. The modified starches may be the potential carriers in the form of hydrogels, similar to the hydrocolloid dressings.

Acknowledgement

The authors gratefully acknowledge the Laboratory of Elemental Analysis and Structural Research at the Faculty of Pharmacy at Wroclaw Medical University for allowing access to DSC, FTIR and PXRD instruments.

Notes

[1] Author contributions: Conceptualization, J.Kobryń and W.Musiał; methodology, J.Kobryń, W.Musiał and T.Zięba; formal analysis, J.Kobryń, M.Rzepczyńska and W.Musiał; investigation, J.Kobryń, W.Musiał, M.Rzepczyńska and T.Zięba; resources, W.Musiał; data curation, J.Kobryń and W.Musiał; writing—original draft preparation, J.Kobryń and W.Musiał; writing—review and editing, J.Kobryń, W.Musiał and T.Zięba; visualization, J.Kobryń, W.Musiał and T.Zięba; supervision, W.Musiał; project administration, W.Musiał; funding acquisition, W.Musiał. All authors have read and agreed to the published version of the manuscript.

[2] Conflicts of interest Conflict of interest: The authors declare no conflict of interest.

References

[1] 

Salman Z.N.; Al-Ani I.; Al Azzam K.M.; Majeed B.J. M.; Abdallah H.H.; Negim El-S. Enhancement of apixaban’s solubility and dissolution rate by inclusion complex (β-cyclodextrin and hydroxypropyl β-cyclodextrin) and computational calculation of their inclusion complexes. ADMET and DMPK (2023). http://doi.org/10.5599/admet.1885.

[2] 

Wang J.; Lu Z.; Wientjes M.G.; Au J.L.S. Delivery of siRNA therapeutics: Barriers and carriers. AAPS Journal 12 (2010) 492-503. http://doi.org/10.1208/s12248-010-9210-4.

[3] 

Marasini N.; Haque S.; Kaminskas L.M. Polymer-drug conjugates as inhalable drug delivery systems: A review. Current Opinion in Colloid & Interface Science 31 (2017) 18-29. http://doi.org/10.1016/j.cocis.2017.06.003.

[4] 

Gaspar R.; Duncan R. Polymeric carriers: Preclinical safety and the regulatory implications for design and development of polymer therapeutics. Advance Drug Delivery Reviews 61 (2009) 1220-1231. https://doi.org/10.1016/j.addr.2009.06.003. https://doi.org/10.1016/j.addr.2009.06.003

[5] 

Khan J.; Alexander Ajazuddin A.; Saraf S. Exploring the role of polymeric conjugates toward anti-cancer drug delivery: Current trends and future projections. International Journal of Pharmaceutics 548 (2018) 500-514. http://doi.org/10.1016/j.ijpharm.2018.06.060.

[6] 

Jung J.; Arnold R.D.; Wicker L. Pectin and charge modified pectin hydrogel beads as a colon-targeted drug delivery carrier. Colloids and Surfaces B: Biointerfaces 104 (2013) 116-121. http://doi.org/10.1016/j.colsurfb.2012.11.042.

[7] 

Saboktakin M.R.; Tabatabaie R.; Maharramov A.; Ramazanov M.A. Synthesis and characterization of superparamagnetic chitosan-dextran sulfate hydrogels as nano carriers for colon-specific drug delivery. Carbohydrate Polymers. 81 (2010) 372-376. http://doi.org/10.1016/j.carbpol.2010.02.034.

[8] 

Parveen S.; Gupta A.D.; Prasad R. Arabinogalactan protein from Arachis hypogaea: Role as carrier in drug-formulations. International Journal of Pharmaceutics 333 (2007) 79-86. http://doi.org/10.1016/j.ijpharm.2006.10.003.

[9] 

Dutta R.K.; Sahu S. Development of oxaliplatin encapsulated in magnetic nanocarriers of pectin as a potential targeted drug delivery for cancer therapy. Research in Pharmaceutical Sciences 2 (2012) 38-45. http://doi.org/10.1016/j.rinphs.2012.05.001.

[10] 

Patani B.; Akin-Ajani O.; Kumaran A.; Odeku O. Irvingia gabonensis (O’Rorke) Bail polymer matrix system for controlled drug delivery. Polymers in Medicine 52 (2022). http://doi.org/10.17219/pim/153521.

[11] 

Schoebitz M.; Ceballos C.; Ciampi L. Effect of immobilized phosphate solubilizing bacteria on wheat growth and phosphate uptake. Journal of Soil Science and Plant Nutrition 13(1) (2013) 1-10. https://doi.org/10.4067/s0718-95162013005000001. https://doi.org/10.4067/s0718-95162013005000001

[12] 

Pandey S.; Malviya R.; Sharma P. Applicability, Commercial Utility and Recent Patents on Starch and Starch Derivative as Pharmaceutical Drug Delivery Carrier. Recent Patents on Drug Delivery & Formulation 9 (2015) 249-256. https://doi.org/10.2174/1872211309666150724101454. https://doi.org/10.2174/1872211309666150724101454

[13] 

Singh N.; Chawla D.; Singh J. Influence of acetic anhydride on physicochemical, morphological and thermal properties of corn and potato starch. Food Chemistry 86 (2004) 601-608. http://doi.org/10.1016/j.foodchem.2003.10.008.

[14] 

Odeniyi M.A.; Ayorinde J.O. Effects of Modification and Incorporation Techniques on Disintegrant Properties of Wheat (Triticum Aestivum) Starch in Metronidazole Tablet Formulations. Polymers in Medicine 44 (2014) 147-155. https://polimery.umw.edu.pl/pdf/2014/44/3/147.pdf

[15] 

Utomo P.; Nizardo N.M.; Saepudin E. Crosslink modification of tapioca starch with citric acid as a functional food. AIP Conference Proceedings 2242 (2020) 040055. http://doi.org/10.1063/5.0010364.

[16] 

Singh J.; Kaur L.; McCarthy O.J. Factors influencing the physico-chemical, morphological, thermal and rheological properties of some chemically modified starches for food applications-A review. Food Hydrocolloids 21 (2007) 1-22. http://doi.org/10.1016/j.foodhyd.2006.02.006.

[17] 

Kapelko-Żeberska M.; Zięba T.; Pietrzak W.; Gryszkin A. Effect of citric acid esterification conditions on the properties of the obtained resistant starch. International Journal of Food Science & Technology 51 (2016) 1647-1654. http://doi.org/10.1111/ijfs.13136.

[18] 

Zięba T.; Szumny A.; Kapelko M. Properties of retrograded and acetylated starch preparations: Part 1. Structure, susceptibility to amylase, and pasting characteristics. LWT - Food Science and Technology 44 (2011) 1314-1320. http://doi.org/10.1016/J.LWT.2010.12.018.

[19] 

Gryszkin A.; Zięba T.; Kapelko-Żeberska M.; Atraszkiewicz A. Hydrothermal modification of wheat starch part 1. Effect of particle size on the viscosity of formed pastes. Journal of Cereal Science 68 (2016) 46-52. http://doi.org/10.1016/j.jcs.2015.10.004.

[20] 

Kobryń J.; Zięba T.; Sowa S.K.; Musiał W. Influence of acetylated annealed starch on the release of β-escin from the anionic and non-ionic hydrophilic gels. Pharmaceutics 12 (2020) 84. http://doi.org/10.3390/pharmaceutics12010084.

[21] 

Zięba T.; Wilczak A.; Kobryń J.; Musiał W.; Kapelko-Żeberska M.; Gryszkin A.; Meisel M. The annealing of acetylated potato starch with various substitution degrees. Molecules 26 (2021) 2096. http://doi.org/10.3390/molecules26072096.

[22] 

Kobryń J.; Raszewski B.; Zięba T.; Musiał W. Modified Potato Starch as a Potential Retardant for Prolonged Release of Lidocaine Hydrochloride from Methylcellulose Hydrophilic Gel. Pharmaceutics 15 (2023) 387, http://doi.org/10.3390/pharmaceutics15020387.

[23] 

Korth C.; May B.C.H.; Cohen F.E.; Prusiner S.B. Acridine and phenothiazine derivatives as pharmacotherapeutics for prion disease. PNAS 98 (2001) 9837-9841. http://doi.org/10.1073/pnas.161274798.

[24] 

Ohlow M.J.; Moosmann B. Phenothiazine: The seven lives of pharmacology’s first lead structure. Drug Discovery Today 16 (2011) 119-131. http://doi.org/10.1016/j.drudis.2011.01.001.

[25] 

Adam K.; Oswald I. The hypnotic effects of an antihistamine : promethazine. British Journal of Clinical Pharmacology 22 (1986) 715-717. https://doi.org/10.1111/j.1365-2125.1986.tb02962.x https://doi.org/10.1111/j.1365-2125.1986.tb02962.x

[26] 

Vaughan G.F.; Leiberman D.M.; Cook L.C. Chlorpromazine in psychiatry. The lancet 265 (1955) 1083-1087. http://doi.org/10.1016/S0140-6736(55)90587-0.

[27] 

Tiwari R.; Srivastava B.; Tiwari G.; Rai A. Extended release promethazine HCl using acrylic polymers by freeze-drying and spray-drying techniques: formulation considerations. Brazilian Journal of Pharmaceutical Sciences 45 (2009). http://doi.org/10.1590/S1984-82502009000400029.

[28] 

Shiotani K.; Uehata K.; Irie T.; Hirayama F.; Uekama K. Characterization of the inclusion mode of β-cyclodextrin sulfate and its effect on the chlorpromazine-induced hemolysis of rabbit erythrocytes. Chemical and Pharmaceutical Bulletin 42 (1994) 2332-2337. https://doi.org/10.1248/cpb.42.2332. https://doi.org/10.1248/cpb.42.2332

[29] 

Tacheva B.; Zheleva A.; Georgieva R.; Tong W.; Gao Ch.; Karabaliev M. Interactions of BSA-nanoparticles with some electroactive drugs. Trakia Journal of Sciences 12(Suppl. 1) (2014) 84-88. http://www.uni-sz.bg/tsj/Vol.%2012%20S1/18.pdf.

[30] 

Banat F.; Al-Asheh S.; Al-Anbar S.; Al-Refaie S. Microwave- and acid-treated bentonite as adsorbents of methylene blue from a simulated dye wastewater. Bulletin of Engineering Geology and the Environment 66 (2007) 53-58. http://doi.org/10.1007/s10064-006-0054-1.

[31] 

El Qada E.N.; Allen S.J.; Walker G.M. Adsorption of Methylene Blue onto activated carbon produced from steam activated bituminous coal: A study of equilibrium adsorption isotherm. Chemical Engineering Journal 124 (2006) 103-110. http://doi.org/10.1016/j.cej.2006.08.015.

[32] 

Rafatullah M.; Sulaiman O.; Hashim R.; Ahmad A. Adsorption of methylene blue on low-cost adsorbents: A review. Journal of Hazardous Materials 177 (2010) 70-80. http://doi.org/10.1016/j.jhazmat.2009.12.047.

[33] 

Guo L.; Li J.; Li H.; Zhu Y.; Cui B. The structure property and adsorption capacity of new enzyme-treated potato and sweet potato starches. International Journal of Biological Macromolecules 144 (2020) 863-873. http://doi.org/10.1016/j.ijbiomac.2019.09.164.

[34] 

Nilsson L.; Bergenståhl B. Emulsification and adsorption properties of hydrophobically modified potato and barley starch. Journal of Agricultural and Food Chemistry. 55 (2007) 1469-1474. http://doi.org/10.1021/jf062087z.

[35] 

Dragan E.S.; Loghin D.F.A. Enhanced sorption of methylene blue from aqueous solutions by semi-IPN composite cryogels with anionically modified potato starch entrapped in PAAm matrix. Chemical Engineering Journal 234 (2013) 211-222. http://doi.org/10.1016/J.CEJ.2013.08.081.

[36] 

Bhattacharyya A.; Banerjee B.; Ghorai S.; Rana D.; Roy I.; Sarkar G.; Saha N.R.; De S.; Ghosh T.K.; Sadhukhan S.; et al. Development of an auto-phase separable and reusable graphene oxide-potato starch based crosslinked bio-composite adsorbent for removal of methylene blue dye. International Journal of Biological Macromolecules 116 (2018) 1037-1048. http://doi.org/10.1016/j.ijbiomac.2018.05.069.

[37] 

Whang T.-J.; Huang H.-Y.; Hsieh M.-T.; Chen J.-J. Laser-induced silver nanoparticles on titanium oxide for photocatalytic degradation of methylene blue. International Journal of Molecular Sciences 10 (2009) 4707-4718. http://doi.org/10.3390/ijms10114707.

[38] 

An C.; Peng S.; Sun Y. Facile Synthesis of Sunlight-Driven AgCl:Ag Plasmonic Nanophotocatalyst. Advanced Materials 22 (2010) 2570-2574. http://doi.org/10.1002/adma.200904116.

[39] 

Tang Y.; Jiang Z.; Tay Q.; Deng J.; Lai Y.; Gong D.; Dong Z.; Chen Z. Visible-light plasmonic photocatalyst anchored on titanate nanotubes: a novel nanohybrid with synergistic effects of adsorption and degradation. RSC Advances 2 (2012) 9406. http://doi.org/10.1039/c2ra21300a.

[40] 

Ebadi A.; Soltan Mohammadzadeh J.S.; Khudiev A. What is the correct form of BET isotherm for modeling liquid phase adsorption? Adsorption 15 (2009) 65-73. http://doi.org/10.1007/s10450-009-9151-3.

[41] 

Coates J. Interpretation of Infrared Spectra A Practical Approach, in Encyclopedia of Analytical Chemistry Meyers R.A., Ed., Wiley Online Library, 2000, pp. 10815-10837. https://doi.org/10.1002/9780470027318.a5606. https://doi.org/10.1002/9780470027318.a5606

[42] 

Ovchinnikov O.V.; Evtukhova A.V.; Kondratenko T.S.; Smirnov M.S.; Khokhlov V.Y.; Erina O.V. Manifestation of intermolecular interactions in FTIR spectra of methylene blue molecules. Vibrational Spectroscopy 86 (2016) 181-189. http://doi.org/10.1016/j.vibspec.2016.06.016.

[43] 

Keshk S.M.A.S.; Al-sehemi A.G. New Composite Based on Starch and Mercerized Cellulose. American Journal of Polymer Science 3 (2013) 46-51. http://article.sapub.org/10.5923.j.ajps.20130303.02.html.

[44] 

Lomelí-Ramírez M.G.; Barrios-Guzmán A.J.; García-Enriquez S.; de Jesús Rivera-Prado J.; Manríquez-González R. Chemical and Mechanical Evaluation of Bio-composites Based on Thermoplastic Starch and Wood Particles Prepared by Thermal Compression. BioResources 9 (2014) 2960-2974. http://doi.org/10.15376/biores.9.2.2960-2974.

[45] 

Ma X.; Liu X.; Anderson D.P.; Chang P.R. Modification of porous starch for the adsorption of heavy metal ions from aqueous solution. Food Chemistry 181 (2015) 133-139. http://doi.org/10.1016/j.foodchem.2015.02.089.

[46] 

Ruland W. X-ray determination of crystallinity and diffuse disorder scattering. Acta Crystallographica 14 (1961) 1180-1185. http://doi.org/10.1107/S0365110X61003429.

[47] 

Ahvenainen P.; Kontro I.; Svedström K. Comparison of sample crystallinity determination methods by X-ray diffraction for challenging cellulose I materials. Cellulose 23 (2016) 1073-1086. http://doi.org/10.1007/s10570-016-0881-6.

[48] 

Al-Ghouti M.A.; Al-Absi R.S. Mechanistic understanding of the adsorption and thermodynamic aspects of cationic methylene blue dye onto cellulosic olive stones biomass from wastewater. Scientific Reports 10 (2020) 15928. http://doi.org/10.1038/s41598-020-72996-3.

[49] 

Bhargav P.B.; Mohan V.M.; Sharma A.K.; Rao V.V.R.N. Structural and electrical studies of sodium iodide doped poly(vinyl alcohol) polymer electrolyte films for their application in electrochemical cells. Ionics 13 (2007) 173-178. http://doi.org/10.1007/s11581-007-0102-2.

[50] 

Hodge R.M.; Edward G.H.; Simon G.P. Water absorption and states of water in semicrystalline poly(vinyl alcohol) films. Polymers 37 (1996) 1371-1376. http://doi.org/10.1016/0032-3861(96)81134-7.

[51] 

Rager T.; Geoffroy A.; Hilfiker R.; Storey J.M.D. The crystalline state of methylene blue: A zoo of hydrates Physical Chemistry Chemical Physics 14 (2012) 8074-8082. http://doi.org/10.1039/c2cp40128b.

[52] 

Farmoudeh A.; Akbari J.; Saeedi M.; Ghasemi M.; Asemi N.; Nokhodchi A. Methylene blue-loaded niosome: preparation, physicochemical characterization, and in vivo wound healing assessment. Drug Delivery and Translational Research 10 (2020) 1428-1441. http://doi.org/10.1007/s13346-020-00715-6.

[53] 

Omer O.S.; Hussein M.A.; Hussein B.H.M.; Mgaidi A. Adsorption thermodynamics of cationic dyes (methylene blue and crystal violet) to a natural clay mineral from aqueous solution between 293.15 and 323.15 K. Arabian Journal of Chemistry 11 (2018) 615-623. http://doi.org/10.1016/j.arabjc.2017.10.007.

[54] 

Angell C.A.; Sare J.M.; Sare E.J. Glass transition temperatures for simple molecular liquids and their binary solutions. Journal of Physical Chemistry 82 (1978) 2622-2629. http://doi.org/10.1021/j100513a016.

[55] 

Taylor L.; Zografi G. Sugar - Polymer Hydrogen Bond Interactions in Lyophilized Amorphous Mixtures. Journal of Pharmaceutical Sciences 87(12) (1998) 1615-1621. https://doi.org/10.1021/js9800174. https://doi.org/10.1021/js9800174

[56] 

Zhou Q.H.; Li M.; Yang P.; Gu Y. Effect of hydrogen bonds on structures and glass transition temperatures of maleimide-isobutene alternating copolymers: Molecular dynamics simulation study. Macromolecular Theory and Simulations 22 (2013) 107-114. https://doi.org/10.1002/mats.201200057. https://doi.org/10.1002/mats.201200057

[57] 

Liu Y.; Bhandari B.; Zhou W. Glass transition and enthalpy relaxation of amorphous food saccharides: A review. Journal of Agricultural and Food Chemistry 54 (2006) 5701-5717. http://doi.org/10.1021/jf060188r.

[58] 

Lin J.; Wang L. Comparison between linear and non-linear forms of pseudo-first-order and pseudo-second-order adsorption kinetic models for the removal of methylene blue by activated carbon. Frontiers of Environmental Science & Engineering in China 3 (2009) 320-324. http://doi.org/10.1007/s11783-009-0030-7.

[59] 

Itodo A.; Itodo H.; Gafar M. Estimation of Specific Surface Area using Langmuir Isotherm Method. Journal of applied science and environmental management 14 (2011) 141-145. http://doi.org/10.4314/jasem.v14i4.63287.

[60] 

Kumar K.V.; Sivanesan S. Prediction of optimum sorption isotherm: Comparison of linear and non-linear method. Journal of Hazardous Materials 126 (2005) 198-201. http://doi.org/10.1016/j.jhazmat.2005.06.007.

[61] 

Azizian S.; Haerifar M.; Basiri-Parsa J. Extended geometric method: A simple approach to derive adsorption rate constants of Langmuir-Freundlich kinetics. Chemosphere 68 (2007) 2040-2046. http://doi.org/10.1016/j.chemosphere.2007.02.042.

[62] 

Bestani B.; Benderdouche N.; Benstaali B.; Belhakem M.; Addou A. Methylene blue and iodine adsorption onto an activated desert plant. Bioresource Technology 99 (2008) 8441-8444. http://doi.org/10.1016/j.biortech.2008.02.053.

[63] 

Kallel F.; Chaari F.; Bouaziz F.; Bettaieb F.; Ghorbel R.; Chaabouni S.E. Sorption and desorption characteristics for the removal of a toxic dye, methylene blue from aqueous solution by a low cost agricultural by-product. Journal of Molecular Liquids 219 (2016) 279-288. http://doi.org/10.1016/j.molliq.2016.03.024.

[64] 

Janus T.; Piechocki J.; Janus A. Acute methemoglobinemia - causes, possible manifestations and treatment. Anaesthesiology & Rescue Medicine 9 (2015) 327-333. https://www.akademiamedycyny.pl/wp-content/uploads/2016/05/201503_AiR_010.pdf (in Polish)

[65] 

Rahman M.A.; Amin S.M.R.; Alam A.M.S. Removal of Methylene Blue from Waste Water Using Activated Carbon Prepared from Rice Husk. The Dhaka University Journal of Science 60 (2012) 185-189. http://doi.org/10.3329/dujs.v60i2.11491.

[66] 

Bakhshi H.; Darvishi A. Preparation and evaluation of hydrogel composites based on starch-g-PNaMA/eggshell particles as dye biosorbent. Desalination and Water Treatment 57 (2016) 18144-18156. http://doi.org/10.1080/19443994.2015.1087344.

[67] 

Guo L.; Li G.; Liu J.; Meng Y.; Tang Y. Adsorptive decolorization of methylene blue by crosslinked porous starch. Carbohydrate Polymers 93 (2013) 374-379. http://doi.org/10.1016/j.carbpol.2012.12.019.

[68] 

Taweekarn T.; Wongniramaikul W.; Boonkanon C.; Phanrit C.; Sriprom W.; Limsakul W.; Towanlong W.; Phawachalotorn C.; Choodum A. Starch Biocryogel for Removal of Methylene Blue by Batch Adsorption. Polymers 14 (2022) 5543. http://doi.org/10.3390/polym14245543.

[69] 

Dang X.; Yu Z.; Yang M.; Woo M.W.; Song Y.; Wang X.; Zhang H. Sustainable electrochemical synthesis of natural starch-based biomass adsorbent with ultrahigh adsorption capacity for Cr(VI) and dyes removal. Separation and Purification Technology 288 (2022) 120668. http://doi.org/10.1016/j.seppur.2022.120668.

[70] 

Junlapong K.; Maijan P.; Chaibundit C.; Chantarak S. Effective adsorption of methylene blue by biodegradable superabsorbent cassava starch-based hydrogel. International Journal of Biological Macromolecules 158 (2020) 258-264. http://doi.org/10.1016/j.ijbiomac.2020.04.247.

[71] 

Chen L.; Zhu Y.; Cui Y.; Dai R.; Shan Z.; Chen H. Fabrication of starch-based high-performance adsorptive hydrogels using a novel effective pretreatment and adsorption for cationic methylene blue dye: Behavior and mechanism. Chemical Engineering Journal 405 (2021) 26953. https://doi.org/10.1016/j.cej.2020.126953. https://doi.org/10.1016/j.cej.2020.126953

[72] 

Tanhaei B.; Ayati A.; Sillanpää M. Magnetic xanthate modified chitosan as an emerging adsorbent for cationic azo dyes removal: Kinetic, thermodynamic and isothermal studies. International Journal of Biological Macromolecules 121 (2019) 1126-1134. https://doi.org/10.1016/j.ijbiomac.2018.10.137. https://doi.org/10.1016/j.ijbiomac.2018.10.137

[73] 

Karaer H.; Kaya Li Synthesis, characterization of magnetic chitosan/active charcoal composite and using at the adsorption of methylene blue and reactive blue4. Microporous and Mesoporous Materials 232 (2016) 26-38. https://doi.org/10.1016/j.micromeso.2016.06.006. https://doi.org/10.1016/j.micromeso.2016.06.006

[74] 

Alijani H.; Beyki M.H.; Kaveh R.; Fazli Y. Rapid biosorption of methylene blue by in situ cellulose-grafted poly 4-hydroxybenzoic acid magnetic nanohybrid: multivariate optimization and isotherm study. Polymer Bulletin 75 (2018) 2167-2180. http://doi.org/10.1007/s00289-017-2148-2.

[75] 

Liu X.; Zhou Y.; Nie W.; Song L. Fabrication of hydrogel of hydroxypropyl cellulose (HPC ) composited with graphene oxide and its application for methylene blue removal. Journal of Materials Science 50 (2015) 6113-6123. http://doi.org/10.1007/s10853-015-9166-y.

[76] 

Sing K.S.W. Reporting physisorption data for gas/solid systems. Pure and Applied Chemistry. 54 (1982) 2201-2218. http://doi.org/10.1351/pac198254112201.

[77] 

Cardenas C.; Latifi A.M.; Vallières C.; Marsteau S.; Sigot L. Analysis of an industrial adsorption process based on ammo-nia chemisorption: Modeling and simulation. Computers & Chemical Engineering 154 (2021) 107474. http://doi.org/10.1016/j.compchemeng.2021.107474.

[78] 

Gordus A.A. Chemical equilibrium: IV. Weak acids and bases. Journal of Chemical Education. 68 (1991) 397-399. http://doi.org/10.1021/ed068p397.

[80] 

Huang Y.; Li S.; Chen J.; Zhang X.; Chen Y. Adsorption of Pb(II) on mesoporous activated carbons fabricated from water hyacinth using H3PO4 activation: Adsorption capacity, kinetic and isotherm studies. Applied Surface Science 293 (2014) 160-168. http://doi.org/10.1016/j.apsusc.2013.12.123.

[81] 

Golachowski A.; Drożdz W.; Golachowska M.; Kapelko-Zeberska M.; Raszewski B. Production and properties of starch citrates—Current research. Foods 9 (2020) 1311. http://doi.org/10.3390/foods9091311.

[82] 

Shen L.; Xu H.; Kong L.; Yang Y. Non-Toxic Crosslinking of Starch Using Polycarboxylic Acids: Kinetic Study and Quantitative Correlation of Mechanical Properties and Crosslinking Degrees. Journal of Polymers and the Environment 23 (2015), 23, 588-594. http://doi.org/10.1007/s10924-015-0738-3.

[83] 

Karma V.; Gupta A.D.; Yadav D.K.; Singh A.A.; Verma M.; Singh H. Recent Developments in Starch Modification by Organic Acids. Starch 74 (2022) 1-14. http://doi.org/10.1002/star.202200025.

[84] 

Kapelko-Żeberska M.; Zięba T.; Singh A.V. Physically and Chemically Modified Starches, in Food and Non-Food Industries Surface Modification of Biopolymers, Thakur Vijay Kumar, Singh Singha Amar, Eds., John Wiley & Sons, Inc., Hoboken, New Jersey, USA,. 2015, pp 173-193. ISBN 978-1-118-66955-6. http://doi.org/10.1002/9781119044901.

Floating objects

Figure 1. Structural models of the adsorbates as: a - starch acetate (SM1), b - starch citrate (SM2), c - starch diphosphate (SM3) and the d - adsorbent methylene blue tautomers (MB).
ADMET-11-1950-g001.jpg
Figure 2. Images of actual appearance (above) and images magnified 10 times with a stereoscopic microscope (SMZ-171-TLED, Motic, Hongkong, China) (below) of A - SM1, B - SM2, C - SM3; petri dish diameter = 10 cm.
ADMET-11-1950-g002.jpg
Figure 3. The FTIR spectra of methylene blue (MB), the pure starches (a) SN, (b) SM1, (c) SM2 and (d) SM3, the physical mixture and the experimental formulation of the starches with adsorbed MB, respectively.
ADMET-11-1950-g003.jpg
Figure 4. The diffractograms of acetylated starch (SM1), starch citrate (SM2) and starch diphosphate (SM3) compared to native starch (SN).
ADMET-11-1950-g004.jpg
Figure 5. The DSC thermograms of methylene blue (MB), the pure starches (SN, SM1, SM2 and SM3), physical mixtures, and the experimental formulations of the starches with adsorbed MB. The subfigures (a,b,c,d) represent thermograms of the first heating cycle and (e,f,g,h) thermograms of the second heating cycle.
ADMET-11-1950-g005.jpg
Figure 6. The DSC thermograms of the starches (SN, SM1, SM2 and SM3). The subfigure (a) represents thermograms of the first heating cycle and (b) the second heating cycle.
ADMET-11-1950-g006.jpg
Figure 7. The plot of MB adsorption on the starch samples with time: (a) SN, (b) SM1, (c) SM2, (d) SM3; • - 2 mg, ◦ -5 mg, ▪ - 10 mg, □ - 25 mg, ▲ - 50 mg, Δ - 125 mg, ♦ - 250 mg, ◊ - 500 mg, - - 750 mg, + - 1000 mg, n = 4, at 22±0.5 °C and 6.0 mg L-1 MB solution with pH 4.26.
ADMET-11-1950-g007.jpg
Figure 8. Comparison of pH values of starch suspensions with adsorbed MB to pure starch suspensions after (a) 1 h and (b) 72 h at 22±2 °C (n = 3).
ADMET-11-1950-g008.jpg
Figure 9. Isotherms of MB adsorbed on the starches: SN, SM1, SM2 and SM3 at 22±0.5 °C and 6.0 mg L-1 MB solution with pH 4.26 (n = 4).
ADMET-11-1950-g009.jpg
Table 1. Number of moles of individual functional groups of modified starches per 1 g of SN.
Modified starchConcentration, mmol g-1
Carbonyl groupsCarboxyl groupsPhosphate groups
SM12.74--
SM2-1.56-
SM3--0.12
Table 2. Isotherm and kinetics models applied for evaluation of obtained data, Cs - concentration of substance in the solution in the equilibrium state (e.s.), qt - adsorbed quantity of adsorbate in time, q -adsorbed quantity of adsorbate in the e.s., qm - maximum monolayer capacity, kF, kL and kBET - adsorption equilibrium constants, k1, k2 - equilibrium rate constants, 1/n - constant, t - time, a - slope, b - intercept, r2 - regression coefficient.
Applied modelGeneral equationParameters
FreundlichADMET-11-1950-i001.jpgADMET-11-1950-i002.jpgb=InkF-r2
LangmuirADMET-11-1950-i003.jpgADMET-11-1950-i004.jpgADMET-11-1950-i005.jpg-r2
BETADMET-11-1950-i006.jpgADMET-11-1950-i007.jpgADMET-11-1950-i008.jpgADMET-11-1950-i009.jpgr2
Pseudo - 1st orderln(q-qt) = lnq - k1tqk1-r2
Pseudo - 2nd orderADMET-11-1950-i010.jpgqk2-r2
Table 3. Composition of crystallinity and amorphousness for SM1, SM2 and SM3 samples compared to SN (n = 3).
Starch typesSNSM1SM2SM3
Crystallinity, %14.3 ± 0.809.8 ± 0.143.2 ± 0.265.7 ± 0.75
Amorphousness, %85.7 ± 0.8090.2 ± 0.1496.8 ± 0.2694.3 ± 0.75
Table 4. Parameters of selected isotherm models for adsorption of 6 mg L-1 MB solution on SN, SM1, SM2 and SM3 starches. A - applies to 2 to 125 mg, B - applies to 250 to 1000 mg of the adsorbents (n = 4).
Isotherm modelParametersSNSM1SM2SM3
ABABABAB
Freundlich1/n0.57231.02544.84420.92212.45033.54912.47691.5960
kF / L g-12.16320.97020.00100.37270.39647.79830.14070.5681
r20.90710.80960.84670.88340.89540.91620.90830.9981
LangmuirkL / L g-10.3020-0.0712-0.15930.0488-0.1671-1.2145-0.1317-0.2738
qm / mg g-18.9767-12.594-0.39207.9177-4.7619-0.4387-3.4807-1.5094
r20.67930.07710.55600.08360.73780.92200.87010.9684
BETkBET(s) / L mg-11.41064.79710.51510.72230.02165.19121.81880.7352
kBET(L) / L mg-10.08210.67680.07410.16660.13991.29430.15390.2591
qm / mg g-13.38220.03180.02900.317527.6760.27301.40690.4535
r20.73310.35820.69070.23950.77060.93340.94340.9813
Table 5. Maximum adsorption capacities (qm) of different starches and other polysaccharides toward MB.
Type of adsorbentqm / mg g-1Ref.
Hydrogel poly(sodium methacrylate) with wheat starch and eggshell1.95[66]
Crosslinked porous corn starch9.46[67]
Starch cryogel of a rice flour and a tapioca starch34.84[68]
Honeycomb biomass adsorbent based on oxidized corn starch-gelatin1551.5[69]
Hydrogel poly(acrylamide) with cassava starch1917[70]
Hydrogel poly(acrylic acid) with potato starch crosslinked with N,N’-methylene-bisacrylamide2967.66[71]
Xanthate modified magnetic chitosan197.8[72]
Chitosan/activated charcoal500[73]
Cellulose-grafted poly 4-hydroxybenzoic acid magnetic nanohybrid7.5[74]
Hydrogel of hydroxypropyl cellulose (HPC) composited with graphene oxide6.59[75]
Native potato starch7.60This work
Acetylated potato starch8.57This work
Diphosphate potato starch16.10This work
Citrate potato starch22.86This work
Table 6. Concentrations of functional groups located on 50 mg of modified starches recalculated on the basis of parameter values of the Henderson-Hasselbalch equation [78] (n = 3).
SM1SM2SM3
pH after 1h6.44 ± 0.055.19 ± 0.095.98 ± 0.07
pKa1*4.763.132.16
pKa2*-4.767.21
pKa3*-6.4012.32
Concentration of functional groups, mmol mg-16.07 ± 1.64 ×10-77.07 ± 2.82 × 10-61.90 ± 0.62 × 10-8

[i] *according to database in LibreTexts™ chemistry [79]


This display is generated from NISO JATS XML with jats-html.xsl. The XSLT engine is libxslt.